Hata analizi ve siyah lekelerin giderilmesi

siyah noktalar nedir?

Siyah lekeler, ürünlerin yüzeyinde koyu veya koyu çizgilerdir., ve kapının yakınında akış yönü boyunca siyah akım çizgisi belirir, hangi bir yüzey kalitesi problemidir, şekilde gösterildiği gibi

Siyah nokta ve siyah şerit

Hata analizi ve siyah lekelerin giderilmesi

1) The melt temperature is too high

If the material temperature is too high, the melt will overheat and decompose, forming carbides. In order to avoid the overheat decomposition of the melt, the temperature at the end of the barrel must be strictly controlled for PVC and other heat sensitive thermoplastic materials. When black spots and stripes are found on the surface of the plastic parts, the temperature controller of the barrel should be checked immediately to see if it is out of control, and the temperature of the barrel and die should be reduced appropriately. Yine de, it should be noted that if the material temperature and die temperature are too low, bright streaks will also appear on the surface of plastic parts.

2) Too large gap of material cylinder

If the wear gap between the screw and the barrel is too large, the converging melt will stay in the barrel, resulting in local overheating decomposition of the retained melt and black spots and stripes. Enjeksiyon kalıplama makinesinin meme deliği çok küçükse veya meme kısmen tıkalıysa, you can first slightly reduce the barrel temperature, observe whether the fault can be eliminated. ikinci olarak, check the barrel, nozzle and die to see if there is any dead angle and smooth grinding.

After taking the above measures, if the fault is not eliminated, the equipment should be repaired in time, and the gap between screw and barrel should be adjusted.

3) Overheat due to friction between melt and die wall

Enjeksiyon hızı çok hızlıysa, the injection pressure is too high, and the relative movement speed between the melt and the cavity wall is too high during mold filling, it is easy to cause friction overheating, which will cause the melt to decompose and produce black spots and wrinkles. Öyleyse, the injection speed and pressure should be reduced appropriately.

4) Poor exhaust of barrel and die

If the cylinder or die is not well vented, the residual gas in the melt will burn due to adiabatic compression, which will cause the melt to overheat and decompose and produce black spots and stripes. Öyleyse, the injection speed can be reduced appropriately, and the exhaust port structure of the barrel can be improved when the particle size and uniformity of the raw material are suitable.

For the poor exhaust of the mold part, check whether the gate position and exhaust hole position are correct, whether the gate type is suitable, remove the rust inhibitor and other volatile substances adhered in the mold, and reduce the amount of mold release agent. On the premise of no flash, the clamping force can be reduced and the exhaust clearance can be increased. Ek olarak, check the barrel and thimble for oil leakage.

5) Bulk coking

When the nozzle does not match with the main channel of the mold, the accumulated material will be coking near the gate and injected into the mold cavity with the flowing material, forming black spots and stripes on the surface of the plastic parts. Öyleyse, the relative position of the nozzle and the main channel of the die should be adjusted in time to make it fit well.

Ek olarak, if the hot runner of the mold is not well designed or manufactured, the molten material will not flow smoothly in the runner, stay and coke, which will also cause black spots and stripes on the surface of the plastic parts. Öyleyse, the surface luminosity of hot runner should be increased and the heating temperature of hot runner should be reduced.

6) Kapıyı doğrudan plastik parçaların üzerine yerleştirmeye uygun olmayan ve kalıplamadan sonra kapıda kalıntı deformasyon oluşturması kolay plastik parçalar için

If the content of volatile matter in raw materials is too high, the drying of water sensitive resin is poor, the amount of recycled materials is too much, the fine powder is too much, the raw materials are not evenly colored, the lubricant type is not selected correctly or used too much, it will lead to black spots and stripes on the surface of plastic parts in varying degrees. Enjeksiyon kalıplama makinesinin meme deliği çok küçükse veya meme kısmen tıkalıysa, we should take corresponding measures according to different situations and eliminate them separately.

 

 

JasonMould Industrial Company Limited Hakkında

Jasonmould bir Çin kalıp üreticisi plastik kalıpların- enjeksiyon kalıbı, döküm kalıpları, plastik şişirme, rotasyonel kalıplama, tıbbi plastik enjeksiyon kalıplama, iki atış plastik enjeksiyon kalıplama, ekleme kalıplama, aşırı kalıplama, metal enjeksiyon kalıplama, mikro enjeksiyon kalıplama, toz enjeksiyon kalıplama, seramik enjeksiyon kalıplama, sıvı enjeksiyon kalıplama, husky enjeksiyon kalıplama, ev kalıp, döküm kalıbı, kalıp aracı, özel kalıplar, Çin kalıpları, hızlı prototipleme araçları, plastik prototipleme araçları, zımba pres takımı, cep telefonu/cep telefonu parçaları için kalıp ve takımlar, Otomotiv parçaları, elektrikli süpürgeler, şarj edilebilir aletler, telefonlar, fotokopi makineleri, bilgisayarlar, multimedya hoparlörler, ve diğer birçok elektronik ürün ve ev aletleri. Ve ayrıca bir plastik ürün üreticisi, kalıp üreticisi Çin- plastik parçalar, plastik su deposu, plastik toplar, plastik konteynırlar, plastik toka, plastik çapa, plastik askı, plastik kaşık, plastik boru bağlantı parçası, plastik takla, plastik sofra takımı, plastik kaplar, plastik şişeler, plastik tepsi, plastik kozmetik konteyner, plastik kasa, plastik yemek kabı, plastik sandalyeler, plastik kapaklar, plastik kapak kapatma, plastik borular, plastik su boruları, plastik düğmeler, plastik boru, plastik yardımcı kutular, plastik raflar ve benzeri.

İletişim:
Kişi: James Yuan
şirket: JasonMould Sanayi Limited Şirketi
Ekle: Uzun Çete Köyü,LongXi Kasabası,BoLuo İlçe,HuiZhou Şehri,Guangdong Eyaleti, Çin